Adhesive Bond Failures: A Guide for Indian Manufacturers

Understanding the failure mode mechanisms of adhesive bonds – how to design robust, durable bonded joints that perform over products lifetime.

How to Identify Adhesive Bond Failures

Adhesive failure is an interfacial bond failure between the adhesive (or coatings, printing inks, sealants) and the adherend. Cohesive failure occurs when a fracture allows a layer of adhesive to remain on both surfaces. Examination of the failure mode provides valuable insights about process variables that affect the strength and durability of the bonded joint, an important consideration for manufacturers in India and other global supply chains. The bonding process involves both adhesive and cohesive forces and failures frequently involve more than one failure mode. Four failure modes are Adhesive failure (interfacial), Cohesive Failure (within adhesive), Substrate Failure (material failure), and Mixed-mode Failure (a combination of adhesive and cohesive failures). Delamination can occur during the manufacture process or at any point during the product's storage or service life. Robust adhesive bonds must possess both bond strength and bond durability. Too often, critical failure mechanisms are not properly identified, and manufacturers end up purchasing unnecessary and costly equipment while chasing a solution.

Types of Adhesive Bond Failure Modes and How They Originate

Adhesion between two materials involves surface science, joint designs, and adhesive (or ink/coating) chemistry. Adhesive joints may fail adhesively or cohesively. The failure mode refers to the mechanism by which an adhesive bond breaks or fails as a result of applied stress or force. When bonds fail, it is critical to identify the underlying causes.

Adhesive joints may fail adhesively or cohesively

Adhesive Failure

Adhesive failures occur at the interface between the adhesive and the adherend (substrate). The adhesive separates cleanly from the substrate. Visually, there will be residual adhesive remaining at any location on only one surface. Adhesive failures almost always originate in the manufacturing process such as foreign contamination, migration of chemical additives into the adhesive bond line, viscosity and thickness attributes of the bonded interface, improper curing, and fluctuations in temperature can generate excessive stress on adhesive bonds due to different thermal expansion properties. The adhesive must properly wet the surface of the substrate or the bond strength will be less than maximum.

Adhesive failures

viscosity

Adhesive Failure

Cohesive Failure

Cohesive failure results in fracture of the adhesive and is characterised by the visual presence of the adhesive material on the matching faces of both adherends (substrates). The bond between the adhesive and the substrates is stronger than the adhesive itself. Cohesive failures that occur in-the-field are typically caused by poor joint design.

Cohesive Failure

Substrate Failure

Substrate Failure (or adherend failure) is the optimal bond strength in which the actual material has broken rather than the bond.

Structural Failure

Mixed-Mode Failure

Mixed-mode failures exhibit characteristics of both adhesion failure and cohesion failure because the interface is partially degraded. Essentially, this failure mode is a transitional phase in which the strength of the adhesive bond is lower than the cohesion failure strength.

Adhesive Versus Cohesive Failure

How to Design Strong Adhesive Bonds for Manufacturing

Adhesive bonds fail for a variety of reasons, including part design, moulding, materials and storage, pretreatment, assembly, and operating field conditions. In today's world of global manufacturing, components are frequently produced in one country and shipped to another for assembly. This protocol alone introduces factors that make bonding more difficult.

Bonding: Critical Process Controls

Why Do Adhesive Bonds Fail?

Adhesive bond failures can occur for a variety of causes, including part design, moulding, materials and storage, pretreatment, assembly, and service conditions. In today's global manufacturing environment, components are routinely made in one country and delivered to another for assembly. This protocol alone introduces factors that make bonding more difficult.

pretreatment

White Papers

In-depth publications and references on adhesion science, surface preparation, and bonding methods.

Solving the Problems of Plastics Adhesion
Science of Solving Plastics Adhesion Problems
Methods for Adhesion Bonding of PPS
Techniques for Measuring Adhesion Bonding
Surface Wetting Pretreatment Methods

Solving the Problems of Plastics Adhesion

Science of Solving Plastics Adhesion Problems

Methods for Adhesion Bonding of PPS

Techniques for Measuring Adhesion Bonding

Surface Wetting Pretreatment Methods

Featured Webinar by Scott Sabreen

In this recorded webinar, you will gain a better understanding of the science behind surface pretreatment of different plastics and learn how to determine the best solutions for your adhesion challenges.

How Polymer Surfaces and Contact Angles Affect Adhesive Bonding

Click each topic to explore the technical details.

Polymer morphology and processing will ultimately affect the ease or difficulty of bonding operations. Semi-crystalline plastics are generally more difficult to bond than amorphous plastics. Acetals, nylons, polyolefins, PPS, polycarbonates, PTFE, and rubber/elastomers present the greatest challenges. Migratory external lubricant sprays, such as silicones, should never be used in moulding facilities because they are carried in the air to all other machines and deposited on moulded parts.

Surface preparation is critical to achieving high adhesive bond strength. Surfaces must be clean and contamination-free from dirt, grease and oils. Low molecular weight materials (LMWM) such as silicones, mould release products and anti-slip agents inhibit bonding. When cleaning plastic surfaces, excess solvent will create weak boundary layers leaving a haze build-up that will inhibit bonding. When using plasma surface pretreatment there are optimal wetting levels — overtreatment and undertreatment must be avoided.

Contact angles and Surface Energy. Understanding the contact angle and its physical properties of interaction between solids and liquids provides valuable information in determining optimal adhesion bonding surface wettability conditions. The higher the surface energy of the solid substrate relative to the surface tension of a liquid (water, printing inks, adhesives, coatings, etc.), the better will be its "wettability," and a smaller contact angle. Contact angles are affected by both changes in surface chemistry and changes in surface topography.

The advancing contact angle is most sensitive to the low energy (unmodified) components of the substrate surface, while the receding angle is more sensitive to the high energy, oxidised groups introduced by surface pretreatments. Thus, the receding angle is actually the measurement most characteristic of the modified component of the surface following pretreatments, as measured using dyne solutions. Therefore it is important to measure both the advancing and receding contact angles on all surface-modified materials.

Let SABREEN's Expertise Benefit Your Company

The SABREEN Group is widely recognised internationally as The Plastics Process Manufacturing Experts. We develop and implement robust process solutions for all types of applications, including extreme environmental reliability. From mission critical zero-defect jet fighter canopy ejection systems to drones, electronics, and underwater structures. SABREEN, with over 40 years of hands-on experience and the author of more than 150 technical publications, offers custom engineered adhesion bonding process solutions. When we work at your site, we bring plasma pretreatment and surface analysis equipment to demonstrate adhesion solutions on your production line.

Design for Manufacturing - The Sabreen Group, Inc.

Bring us your toughest adhesion challenges

Call us today to discuss your application and SABREEN's solutions, pro bono.

Request Your Free Quote


Request your free quote

Scott Sabreen — President and Chief Engineer, with over 30 years of expertise. Contact us today to discuss your application and SABREEN solutions free of charge and with no obligation. Bring us your most difficult challenges.

Phone: +1 972-820-6777

Contact us →

Frequently Asked Questions

What is the first thing to check when a bond fails in production but passed in development?

What changed on the surface. Development parts are typically clean, recently moulded and handled carefully; production parts carry mould release, handling residues, longer storage after treatment and possibly a different resin lot. The adhesive and the process are usually the last things to have changed, and they are usually where people look first.

What does the failure surface tell you?

A great deal. Adhesive left cleanly on one substrate points to inadequate surface preparation on the other. Adhesive split through its own thickness points to the adhesive being the weakest element rather than the interface. Substrate material pulled away with the adhesive indicates the bond was stronger than the part. Reading the failure surface directs the corrective action.

Can a bond be too strong?

It can be inappropriate. Where a joint is intended to fail in a controlled way -- for access, for serviceability or for safety -- a bond stronger than the substrate moves the failure into the part itself. The design target is a defined failure mode, not maximum strength.

How do environmental conditions cause a bond to fail over time?

Temperature cycling, humidity, chemical exposure and UV all attack a bonded joint, and they attack the interface before they attack the bulk adhesive. A joint that passes on the day it is made can fail months later through hydrolytic attack at the interface, which is why durability testing needs to reflect service conditions rather than just measuring initial strength.

Scott Sabreen

Scott Sabreen
President & Chief Engineer
30+ Years of Expertise

Describe your problem in two sentences. Scott Sabreen replies personally, usually within one business day.

Submission Successful!

Thank you. Scott has your message and will reply by email, usually within one business day.

We Have Received Your Request

We have received your request and will be in touch shortly.

🌐 India (English) ▴