Carbon Black Selection for Successful Through Transmission Laser Welding and Joining

Abstract

Laser welding is used in a wide range of applications to join thermoplastics because it is a noncontact heating method with short cycle times and lower cost. For both surface heating and through transmission heating, carbon black is the most frequently used colourant. It was found that carbon black types with low particle aggregation and distribution were most effective for laser heating. Experiments with laser line beam scanning showed that a slight tilt in the laser head could produce different heating when traveling forward as compared to backward. For dissimilar polymer joining, it was found that surface texturing increased the adhesion joint area and the amount of mechanical interlocking, resulting in superior joints.

Key Takeaways

  • Carbon black type matters, not just weight percent. Most literature ignores the distinction; absorption and heat conversion vary greatly.
  • Low particle aggregation and distribution proved most effective for laser heating.
  • Typical loading is 0.1% to 1% by weight, and in ABS joining 0.1% was the most effective level.
  • Carbon black is not soot. Soot is what forms when a substance burns incompletely; they are very different materials.
  • Laser travel direction changes the result. A slight tilt in the laser head heats differently forward versus backward.

Frequently Asked Questions

Does the type of carbon black really matter for laser welding?

Yes, considerably. Most laser heating literature discusses only the weight percent, but different carbon black types vary greatly and influence both the absorption of laser energy and its conversion into heat. Types with low particle aggregation and distribution were found most effective.

How much carbon black should be added?

Typically 0.1% to 1% by weight is an effective way to incorporate a laser absorber into one of the parts. In through-transmission joining of ABS to PTFE/PET films, 0.1% by weight proved most effective because it produced thicker layers exceeding the glass transition temperature, letting the ABS flow and improving adhesion.

What is the difference between carbon black and soot?

They are very different substances. Soot forms when a polymer or other substance burns incompletely and is generally amorphous. Carbon black is a manufactured material with controlled structure, and that control is what makes its laser absorption behaviour predictable.

Does surface texturing help laser joining?

Yes. Texturing the ABS surface to produce ridges or crosshatching showed promising results, because the textured surface has a larger area and increases mechanical interlocking at the interface — particularly useful for joining dissimilar polymers.

Why would laser travel direction affect weld quality?

Experiments with laser line beam scanning showed that a slight tilt in the laser head produces different heating traveling forward, in the pull direction, compared with traveling backward. It is a setup variable worth checking when weld quality varies along a joint.

Introduction

Laser welding of thermoplastics can be achieved using two different heating methods: surface heating and through transmission heating [1-5]. For both surface heating and through transmission heating, a colourant is added to the polymer for laser absorption. Carbon black is the most frequently used colourant, but most of the literature on laser heating of polymers does not discuss the different types of carbon black. Therefore, in this work, we will review the different types of carbon black and their laser absorption performance. In addition, the effects of surface texturing and laser travel direction on joining also will be discussed in an experimental study of laser joining of ABS.

Laser Heating

As mentioned earlier, laser heating is possible with both surface heating and through transmission heating [5]. As shown in Figure 1, surface heating can be accomplished by expanding the laser beam and simultaneously heating the surfaces of both parts using mirrors. It also is possible to use a laser line beam or laser spot with a scanning mirror to rapidly scan and heat the surfaces of the parts, as shown in Figure 2. In either case, an absorber, such as carbon black, needs to be incorporated into the plastic part for laser absorption and heating.

For through transmission laser heating, one part is transparent to the laser while the second has an additive, such as carbon black, to absorb the laser radiation and convert it into heat (Figure 3). There are multiple ways to use through transmission laser heating. In scan heating, the laser beam scans the joint lines by either moving the laser or using scanning mirrors (Figure 4). For simultaneous heating, the laser beam is either expanded or multiple laser sources are used in conjunction with optical fibre bundles to simultaneously heat the whole joint area (Figure 5). In quasi-simultaneous heating, a high-speed scanning mirror is used to rapidly scan the joint area, simulating simultaneous heating using a single, high-power laser beam (Figure 6). Another option is to use simultaneous heating with masking to only heat the joint area while blocking the laser beam from reaching other areas (Figure 7). Here too, the absorbing part includes a colourant, such as carbon black, to absorb and convert the laser radiation into heat.

Carbon Black

For many applications, adding small amounts of carbon black (typically ranging from 0.1 percent to 1 percent by weight) is an effective way of incorporating a laser absorber into one of the plastic parts. Usually, the type of carbon black that is used in not considered – just the weight percent [6]. However, the different types of carbon black vary greatly, and they can influence the absorption and conversion of laser energy into heat.

First, it is important to recognise that carbon black and soot are very different substances. Soot forms when a polymer or other substance is not burnt completely. Soot is generally an amorphous carbon in powder form with much lower surface area than carbon black. Carbon black is produced from incomplete burning of heavy petroleum products followed by extraction of organic compounds, resulting in over 97 percent elemental carbon. As shown in Table 1, carbon black is frequently categorised based on the manufacturing process [7]. Carbon black types that have low particle aggregation and distribution were most effective for laser heating.

The combination of carbon black type together with weight percent of carbon black in the polymer will influence the laser absorption. For a given carbon black type, using lower weight percentages (0.1 percent or 0.15 percent) of carbon black results in partial transmission into the part, yielding sub-surface heating. This is beneficial when thicker melt layers are needed without surface degradation. Alternatively, when using high weight percentages (0.5 percent and higher), most of the absorption is near the surface, which results in thinner melt layers.

Through Transmission Laser Joining of ABS

Experiments evaluating the laser joining of ABS to PTFE/PET films were performed using laser line beam scans. ABS plaques were moulded with different types and levels of carbon black. It was found that using 0.1 percent weight carbon black was most effective for this application because it produced thicker layers that exceeded the glass transition temperature (Tg). This allowed the ABS to flow more readily and improved adhesion to the PTFE/ PET film.

Texturing of the ABS surface to produce ridges or crosshatching showed promising results (Figure 8). The textured surface had a larger area, and it increased the mechanical interlocking at the interface. Manual peel strength felt generally high, especially when peeling perpendicular to the ridges. Visual inspection of these joints was very promising, showing extensive amounts of cohesive failure in the PTFE/PET film (Figure 9).

Heating of the ABS was done using a Leister 800 laser line beam head mounted on a Fanuc robot. The laser head was slightly tilted in one direction so that the intensity is slightly different when traveling in one direction versus the opposite direction, referred to as push and pull directions, as shown in Figure 10. To evaluate the effect of the tilt, a Pico Technology USB TC-08 thermocouple data logger was used to measure the temperature history during push-pull heating.

As shown in Figure 11, the temperature in the push direction is significantly lower than in the pull direction. Similarly, the temperature also was measured for push-push (Figure 12) and pull-pull (Figure 13). In both cases, the temperature variation between passes was smaller, and pull-pull resulted in slightly higher surface temperatures. In general, the temperatures that were measured were lower than expected, probably because the thermocouples were large and just placed on top of the surface. Using smaller thermocouple wires and pressing the tip into the ABS surface with a heated tool would improve the measurement accuracy.

Conclusion

Laser heating for welding and joining of thermoplastics was studied to determine the effects of carbon black type and content level, surface texturing and laser travel direction on joint quality. For both surface heating and through transmission heating, carbon black is the most frequently used colourant. It was found that carbon black types that have low particle aggregation and distribution were most effective for laser heating. Experiments with laser line beam scanning with ABS showed that a slight tilt in the laser head could produce different heating when traveling forward (or pull direction) as compared to backward (or push direction). For dissimilar polymer joining of ABS to PTFE/PET film, it was found that surface texturing increased the adhesion joint area and the amount of mechanical interlocking, resulting in superior joints.

References and Acknowledgements

  • J. Schulz and E. Haberstroh, “Welding of Polymers Using a Diode Laser,” SPE ANTEC Proceedings, 2000.
  • H. Ponte, J. Korte, “Laser Butt Welding of Semi-Crystalline Thermoplastics,” SPE ANTEC Proceedings, 1996.
  • V.A. Kagan and G.P. Pinho, “Laser Transmission Welding of Semi-Crystalline Thermoplastics Part II: Analysis of Mechanical Performance of Welded Nylon,” SPE ANTEC Proceedings, 2000.
  • M. Rhew, A. Mokhtarzadeh and A. Benatar, “Through Transmission Laser Welding of Polycarbonate and HighDensity Polyethylene,” SPE ANTEC Proceedings, 2003.
  • D. Grewell, A. Benatar and J. Park, Editors, Plastics and Composites Welding Handbook, Hanser, 2003.
  • B. Acherjee, A.S. Kuar, S. Mitra and D. Misra, “Effect of carbon black on temperature field and weld profile during laser transmission welding of polymers: A FEM study,” Optics & Laser Technology 44 (2012) 514–521.
  • Orion Engineered Carbon LLC company literature.

We would like to thank Leister Corp. for use of the laser beam scanner, Fanuc America for use of the robot and Kimastle Corp. for its automation cell.

Avraham (Avi) Benatar is an associate professor of welding engineering and director of the Plastics and Composites Joining Laboratory. He also is the coordinator of the Welding Engineering Distance Education Master of Science program and the faculty director of the College of Engineering Master of Global Engineering Leadership. He earned the S.B., S.M and Ph.D. degrees in Mechanical Engineering from the Massachusetts Institute of Technology.

Scott R. Sabreen is founder and president of The Sabreen Group, Inc., an engineering company specialising in secondary plastics manufacturing processes – laser marking, surface pretreatments, bonding, decorating and finishing, and product security. Sabreen has been developing pioneering technologies and solving manufacturing problems for more than 30 years. He can be contacted at 972.820.6777 or by visiting www.sabreen.com or www.plasticslasermarking.com.


Request your free quote

Scott Sabreen — President and Chief Engineer, with over 30 years of expertise. Contact us today to discuss your application and SABREEN solutions free of charge and with no obligation. Bring us your most difficult challenges.

Phone: +1 972-820-6777

Contact us →

Scott Sabreen

Scott Sabreen
President & Chief Engineer
30+ Years of Expertise

Describe your problem in two sentences. Scott Sabreen replies personally, usually within one business day.

Submission Successful!

Thank you. Scott has your message and will reply by email, usually within one business day.

We Have Received Your Request

We have received your request and will be in touch shortly.

🌐 India (English) ▴