Dual-Purpose ‘Laser Additives’ Drive Marking and Welding of Polymers

Dual-purpose laser additives blended into polymers during primary processing allow for marking and transmission welding of clear and opaque polymers. Novel chemical additives, including those that are FDA-/medical-compliant, achieve high-strength hermetic seal weld joints and indelible opaque marking contrast. Laser marking and laser welding processes are noncontact, easy to control and eco-friendly. Designed for affordable, high-speed lasers and equipment, marking and welding of polymers meet the challenges of today’s complex applications.

Key Takeaways

  • One compound, two processes. Dual-purpose additives support marking and through-transmission welding in the same material.
  • TTLW runs in three stages — heating, melding and welding — with typical weld times of one to eight seconds.
  • The two parts need opposite optical properties: the top must transmit the wavelength, the bottom must absorb it in a thin layer.
  • Mid-range absorption is the worst case, heating the whole thickness and making a part a poor candidate for either side of the joint.
  • Laser welding delivers hermetic seals with no flash, no particulates, minimal heat-affected zone and no marring of the part surface.

Frequently Asked Questions

What does “through transmission” mean in laser welding?

The laser passes through the laser-transparent upper part and is absorbed at the surface of the laser-absorbent lower part. Parts are pre-assembled and clamped so the joining surfaces are in intimate contact, and the weld forms at that interface.

What are the stages of a through-transmission laser weld?

Three. In the heating stage the laser heats the absorbent polymer at the interface, which expands and raises weld pressure. In the melding stage further expansion increases pressure and a small amount of welding occurs. In the welding stage sufficient molten material collapses to form a real weld, typically on the order of 0.13 mm.

Can glass-filled materials be laser welded?

Filled materials have been welded with up to 50% glass, but not for hermetic seals. Fillers, additives and pigments all alter how a polymer responds to the laser beam, so material suitability is more sensitive with laser welding than with any other joining process.

Why choose laser welding over ultrasonic or hot plate welding?

It is non-contact with light clamping under a smooth glass plate, so nothing mars the part and no vibration is transmitted. The weld is subsurface and nearly invisible, the heat-affected area is very small so fragile pre-placed components survive, there is no flash to trim, and hermetic gas-tight seals are achievable.

Can dissimilar plastics be laser welded together?

Yes, provided they meet the necessary optical and thermal criteria. Each polymer transmits the three principal welding wavelengths differently, so both materials need evaluating together rather than individually.

Product Applications

Clear, semi-transparent and opaque coloured polymers, including nylons, polyethylene terephthalate (PET), polycarbonates, polyolefins, polyvinyl chloride (PVC), styrenics and thermoplastic elastomers (TPUs) and thermoplastic polyurethanes (TPEs), are uniquely formulated using non-heavy metal, FDA-/European Food Safety Authority (EFSA)-approved additives to achieve high-contrast marking quality, including laser welded products (Figure 1). Polymer clarity, spectral transmission and base physical properties are not affected. Noncontact digital laser marking replaces expensive adhesive labels and ink-chemical printing processes. The result is a cost-effective, environmentally friendly and superior aesthetic appeal.

Laser Marking Surface Reaction Mechanisms

The advancements achieved in formulating laser chemical additives for use with near-infrared (NIR) lasers (1,060-1,080nm wavelength) include their compatibility with ytterbium fibre, vanadate and Nd:YAG lasers. Most polymers do not possess NIR absorption properties without chemical additives. Polymers that can be marked by lasers are those that absorb laser light and convert it from light energy to thermal energy. Additives, fillers, pigments and dyes are used to enhance the absorption of laser energy for localised colour changes. Vastly different formulation chemistries and laser optics/setup parameters are configured depending upon the desired marking contrast and functionality.

Two common surface reaction mechanisms are shown in Figure 1. First, thermal chemical “carbonisation” or “charring” can occur, where the energy absorbed in the substrate raises the local temperature of the material surrounding the absorption site high enough to cause thermal degradation of the polymer. The darkness or lightness of the mark is dependent on the energy absorbed, as well as the material’s unique thermal degradation pathway. By optimising the laser setup, there is minimal surface carbonisation residue.

A second surface reaction, “foaming,” is a chemical change effected through use of additives that release steam during degradation, resulting in foaming of the polymer. During the foaming process, the laser energy is absorbed by an additive that is in close proximity to the foaming agent. The heat from the absorber causes the foaming agent to degrade, releasing steam. Through tight control of the laser-operating parameters, high-quality and durable light-coloured “white” marks can be generated on dark substrates.

A third reaction, laser energy (not shown), is used to heat/degrade one colourant in a colourant mixture, resulting in a colour change. An example is a mixture of carbon black and a stable, inorganic colourant. When heated, the carbon black is removed, leaving behind the inorganic colourant. These mixed colourant systems are dependent on specific colourant stabilities, and not all colour changes are possible. Carbon black formulations are integral in laser welding.

Laser Additive Chemistries for Marking and Welding

Near-infrared laser additives improve the degree of contrast, which can be further intensified by changing the laser setup parameters. Polymers possess inherent characteristics to yield “dark-coloured” or “light-coloured” marking contrast. Some colourant compounds containing low amounts of titanium dioxide (TiO2) and carbon black also absorb laser light and can improve marking contrast. Each polymer grade, even within the same polymeric family, can produce different results. Additive formulations cannot be toxic or adversely affect the products’ appearance, physical or functional properties.

Compared to ink printing processes (pad/screen printing and inkjet), laser additives are cost-saving and can demonstrate 20 percent and faster marking speeds vs. non-optimised materials. Laser additives are supplied in pellet granulate and powder form. Granulate products can be blended directly with the polymer resin, while powder forms are converted to masterbatch. Most are easily dispersed in polymers. Based upon the additive and polymer, the loading concentration level by weight (in the final part) ranges between 0.01 and 4.0 percent.

Both granulate and powder form can be blended into pre-compounded colour material or colour concentrate. The selection of which additive to incorporate depends upon the polymer composition, substrate colour, desired marking contrast colour and end-use certification requirements. For extrusion, injection moulding and thermoforming operations, pre-colour compounded materials vs. colour concentrate yields better uniformity. Hand-mixing should be avoided. Mould flow and gate type/location are important factors. Homogeneous distribution/dispersion of laser additives throughout each part is critical to achieve optimal marking performance.

Some additives contain mixtures of antimony-doped tin oxide and antimony trioxide that can impart a “grayish” tint to the natural (uncoloured) substrate opacity. Other additives can contain aluminium particles, mixed metal oxides and proprietary compounds. Colour adjustments are made using pigments and dyes to achieve the final colour match appearance. As commercially supplied, specific additives (also used for laser welding) have received FDA approval for food contact and food packaging use under conditions A-H of 21 CFR 178.3297 – Colourants for Polymers. For the European Union, there are similar compliance statements. Certification conditions are specific for polymer type, loading level threshold and direct or indirect contact. Further qualification of FDA-approved additives blended into a “final part” can achieve biocompatibility of medical devices.

During the laser additive loading/colour match chemistry, it is not uncommon for a finished product to contain less laser additive than the calculated amount. This problem almost always relates to nonuniform distribution during extrusion or moulding. Simple adjustments to the moulding machine, such as increasing the back pressure and screw rotation speed, will resolve most issues. Homogeneous distribution/dispersion of laser additives throughout each part is critical to achieve optimal marking performance. For extrusion, injection moulding and thermoforming operations, precolour compounded materials vs. colour concentrate yields better uniformity. Hand-mixing should be avoided. Mould flow and gate type/location are important factors.

Principles of Through Transmission Laser Welding

The term “through transmission” derives from the fact that the laser passes through the laser-transparent upper part to the surface of the laser-absorbent lower part, as depicted in Figure 2. Three stages are involved in Through Transmission Laser Welding (TTLW) of plastics. In TTLW, the parts are pre-assembled and clamped together to provide intimate contact between their joining surfaces. In this article, high-power diode lasers (?= 800-1,000nm) and solid-state lasers (Ytterbium fibre and Nd:YAG laser, ?=1,060-1,080nm) are utilised.

During the heating stage, the laser energy heats the laser-absorbent polymer at the interface, causing the part to expand, which increases the weld pressure. At the focus of the beam, the laser power is at its maximum and the part begins to melt at that point, creating a melt zone. This is the start of the second stage, the melding stage. Further expansion of the parts takes place, creating additional expansion with a corresponding increase in pressure. At this point, a small amount of welding has taken place.

The welding stage is the final stage. Sufficient molten material is generated to create a real weld. There is a collapse of the melted material, similar to that of hot plate or fusion welding. For most applications, this is on the order of 0.13mm (0.005?). Typical weld times are on the order of one to eight seconds for most applications, although larger parts can run longer. There are four principal TTLW laser welding processes: contour, mask, simultaneous and quasi-simultaneous welding.

The two parts to be welded must have different optical absorption properties at a given weld length. The top, laser-transparent part must transmit as much of the wavelength as possible while the bottom, laser absorbent part must absorb as much as possible in a thin layer. This results in the most energy-efficient combination because a high amount of energy is absorbed at the interface and it can degrade the top part before the bottom part is soft enough to weld. Excessive reflectivity also causes an increase in the amount of energy that is needed for welding.

Material suitability is more sensitive with laser welding than with any other joining process. Laser welding can theoretically weld all thermoplastics that are transparent to the laser beam. However, each polymer’s ability to transmit light from lasers of the three principle wavelengths used in laser welding is different. Furthermore, the response of a given polymer to laser beams will be altered by the presence of fillers, additives and pigments.

Materials with high absorption rates are ideal for the lower part in TTLW welding because they absorb most of the energy at the weld interface and create a thin, heated surface layer that is ideal for laser welding. Materials with absorption rates in the middle ranges can be a problem because they absorb the laser energy through the thickness of the material, and that results in heating of the whole material thickness. These materials allow very little energy through; therefore, they are poor candidates for the top material in TTLW laser welding. Furthermore, they do not absorb very much energy at their top edge and, consequently, make a poor selection for the lower material. Filled materials have been welded with up to 50 percent glass, but not for hermetic seals.

Principle advantages of TTLW include the following:

  • Noncontact welding. Laser welding uses a smooth glass plate to hold the parts to be welded with a light clamping force of 100lbs or less, and there is no contact with the welding instrument. Consequently, there is nothing to mar the surface of the welded parts, and there is no welding pressure required that could damage delicate parts.
  • Subsurface welding. The weld occurs at the interface between the two parts. The weld is nearly invisible with transparent parts and completely invisible with opaque parts. The weld can be just below the surface or deep in the parts.
  • Precise welding. The size and location of the laser weld can be very precise, and no vibration is transmitted to the part to be welded. For those versions of the process that require relative motion between the laser and weldments, it is the laser that moves. Consequently, laser welding is the most precise of the welding processes.
  • Minimal heat-affected area. The weld spot is very small and the heat-affected area is quite contained. As a consequence, it is possible to weld very close to other components without affecting them, permitting welding of subassemblies with sensitive and fragile parts previously emplaced. Furthermore, distortion and degradation due to heat are extremely limited, and residual stress is reduced.
  • Ability to weld dissimilar plastics. Dissimilar plastics that meet the necessary criteria can be welded to each other.
  • No flash. In laser welding, the weld is totally enclosed and no flash is created that must be trimmed off. There are no loose particulates.
  • Hermetic seals. Laser welding is capable of creating a hermetically sealed, gas-tight weld.
  • Energy efficiency. Relative to other welding processes, laser welding is highly energy efficient. This also means no excess heat is generated that must be removed from the workplace.

Conclusion

Dual-purpose laser additives incorporated into polymers yield superior marking contrast, line edge detail and speed. These additives optimise laser welding of similar and dissimilar thermoplastics. Advancements in affordable fibre laser technology have been instrumental. These benefits rapidly offset the incremental material additive cost. Optimised material-science chemistry for laser marking and welding requires expertise in polymers, colourants, pigments and dyes relative to solubility, particle sizes, threshold concentration limits, colour match and regulatory certifications (GRAS, FDA Direct/Indirect Food Contact). Laser marking and TTLW of polymers meet the challenges of today’s applications.

References

  • Scott R. Sabreen, “FDA-Approved Additives Boost Inline Laser Marking,” Plastics Decorating Magazine, April/May 2015
  • Jordan Rotheiser, specialist consultant for The Sabreen Group Inc. Welding excerpts from Joining of Plastics, Handbook for Designers and Engineers, Third Edition, Jordan Rotheiser, Carl Hanser Verlag, Munich, 2009

Scott R. Sabreen is founder and president of The Sabreen Group, Inc., an engineering company specialising in secondary plastics manufacturing processes ? laser marking, surface pretreatments, bonding, decorating and finishing, and product security. Sabreen has been developing pioneering technologies and solving manufacturing problems for more than 30 years. He can be contacted at 972.820.6777 or by visiting www.sabreen.com or www.plasticslasermarking.com.


Request your free quote

Scott Sabreen — President and Chief Engineer, with over 30 years of expertise. Contact us today to discuss your application and SABREEN solutions free of charge and with no obligation. Bring us your most difficult challenges.

Phone: +1 972-820-6777

Contact us →

Scott Sabreen

Scott Sabreen
President & Chief Engineer
30+ Years of Expertise

Describe your problem in two sentences. Scott Sabreen replies personally, usually within one business day.

Submission Successful!

Thank you. Scott has your message and will reply by email, usually within one business day.

We Have Received Your Request

We have received your request and will be in touch shortly.

🌐 India (English) ▴