Fibre Laser Marking on Nylon (Polyamide) Plastics

The demand for high-contrast laser marking on nylon (polyamide) plastic products is rapidly increasing due to its wide range of industrial applications. Functional and decorative markings include alphanumeric identification, data matrix/QR vision codes, diagrams and micro-structures.

Polyamides, including Polyphthalmides (PPA), are among the most challenging polymers to laser mark due to their diverse material properties, moulding conditions and laser configurations. Smart additives for near-infrared lasers solve marking contrast problems and increase marking speed (faster cycle time) without affecting material properties.

This article provides an understanding of nylons, chemical additives and fibre lasers to achieve high-contrast colour and economical laser marking operations.

Key Takeaways

  • Polyamides including PPA are among the hardest polymers to mark, given their diverse properties, moulding conditions and laser configurations.
  • Contrast is not only colour change — variable light diffraction contributes, alongside fine-line resolution and sharpness.
  • Substrate colour is a variable in itself, since carbon black, TiO2 and flame retardants all absorb laser light differently.
  • Fibre lasers focus below 20 microns, giving the high energy density that fine nylon marking requires.
  • MOPA at 20–50 ns is the effective window for superior contrast colour on most polymers.
Photo 3. Laser marking on resin-rich moulded nylon surface, 30% glass-filled.

A basic parameter for describing the quality of marking is the colour contrast between the marked surface and the substrate. There are three surface mechanisms for colour change using NIR lasers, including Ytterbium fibre, Vanadate (Nd:YVO4) and Nd:YAG: 1) black marking by carbonisation, 2) white marking by foam generation and 3) colour changes by laser-induced thermal chemical reactions of pigmented polymers¹. Among the most demanded contrast colours are opaque white on black, jet black on white and opaque white on medium blue. These colour combinations often require chemical additives. Additives improve the degree of colour contrast (absorption of laser light), which are further intensified by optimal laser selection and marking parameters.

Frequently Asked Questions

What makes nylon difficult to laser mark?

Polyamides, including polyphthalamides, have diverse material properties, moulding conditions and laser configurations, and like most polymers they do not inherently absorb laser light — which prevents the colour change that forms a mark. Laser-enhancing additives are what solve contrast, speed and durability.

How is marking quality judged, beyond contrast?

By fidelity — fine-line resolution and sharpness. Contrast itself is not always achieved by colour change alone, since variable light diffraction also contributes, so both aspects need assessing together.

Does the colour of the nylon affect marking?

Yes. Substrate colour is a genuine factor because compounds such as carbon black, titanium dioxide and flame retardants each possess varying degrees of laser light absorption, which changes how the material responds.

Why did ytterbium fibre lasers replace YAG for this work?

They entered the industrial marking market around 2010 offering superior beam quality and high brightness, focusing to a spot below 20 microns for high energy density. They are also versatile, cost effective and effectively plug-and-play with near-zero maintenance.

What pulse width range works best?

Variable short-pulse MOPA fibre lasers in the 20 to 50 ns range are exceptionally effective for achieving superior contrast colour on most polymers, nylons included. Q-switched fibre lasers at 100 to 150 ns are limited to around 80 kHz repetition rate.

What Is Nylon (Polyamide)?

Polyamides, or nylon, are the major engineering and high-performance thermoplastics class containing repeating amide linkages, i.e., –CO-NH–. These are is formed by condensing identical units, copolymers for different units. Nylon is made from polycondensation of diacid with a diamine or by ring-opening polymerisation of lactams with six, 11 or 12 carbon atoms². Nylon monomers can be aliphatic, semi-aromatic or aromatic (aramids) and can range in structure from amorphous, semi-crystalline and of greater or lesser crystallinity.

The aliphatic polyamides are produced on a much larger scale than the fully aromatic polyamides and are one of the most important class of engineering thermoplastics. Nylon laser marking colour contrast on 20% glass-fill, matte surface texture are amorphous or only moderately crystalline when injection moulded, but the degree of crystallinity can be increased.

Two important polyamides are poly(hexamethylene adipamide) (nylon 6,6) and polycaprolactam (nylon 6). Additional aliphatic polyamides include nylon 12, 69, 6-10, 6-12, 46 and 1212. Nylon 11 is a bio-based engineering plastic that is derived from renewable resources (castor plants).

Semi-aromatic, semi-crystalline polyamides made from the condensation of aliphatic amides include PA 6T & PA 6I. Semi-aromatic polyamides often are a cost-effective alternative to the more expensive fully aromatic aramids. Aromatic polyamides, called aramids, have higher strength, better solvent-, flame- and heat-resistance and greater dimensional stability than aliphatic amides. A commonly recognised aromatic amide is Kevlar, poly(p-phenylene terephthalamide).

Polyamides, including Polyphthalmides (PPA), are among the most challenging polymers to laser mark due to their diverse material properties, moulding conditions and laser configurations.

Polyphthalamide (PPA) is a subset of thermoplastic synthetic resins in the polyamide (nylon) family, defined as when 55% or more moles of the carboxylic acid portion of the repeating unit in the polymer chain is composed. PPA is semi-aromatic, semi-crystalline. PPAs fill the performance gap between aliphatic nylons, such as PA6,6 and PA6, and the much more expensive polyaramids.

"Smart" Additives

One parameter for describing the quality of marking is the colour contrast between the marked surface and the background. Contrast is not always achieved by the colour change itself, as it also can be obtained by the variable light diffraction.

Equally important is marking quality and/or fidelity, i.e., fine-line resolution or sharpness. Many polymers, including nylons, do not inherently absorb laser light, which prevents colour change. Laser-enhancing chemical additives significantly improve marking contrast, speed and durability (see Image 1). Substrate colour is a factor since compounds like carbon black, TiO2 and flame retardants possess varying degrees of laser light absorption.

Laser additives are supplied in pellet granulate and powder form. Granulate products are blended directly with the polymer resin, while powder forms are converted to masterbatch. The loading concentration level by weight (in the final part) typically ranges between 0.01 and 3.0%. Homogeneous distribution/dispersion of laser additives throughout each part is critical to achieve optimal colour contrast.

Some additives contain mixtures of antimony-doped tin oxide and antimony trioxide that can impart a “grayish” tint to the natural (uncoloured) substrate opacity. Other additives can contain aluminium particles, mixed metal oxides and proprietary compounds.

Colour adjustments are made using pigments and dyes to achieve the final colourmatch appearance. Specific additives have received FDA approval for food contact and food packaging use under conditions A-H of 21 CFR 178.3297 Colourants for Polymers¹.

Ytterbium Fibre Lasers

NIR Ytterbium fibre lasers entered the industrial marking market in the 2010 timeframe, replacing traditional YAG lasers. Fibre lasers possess superior beam quality (M2) and high-brightness and can focus to a small spot size (less than 20 microns), which leads to high energy density. Fibre lasers are extremely versatile, cost effective and plug-and-play with near zero maintenance.

Fixed-pulse (Q-switched) and variable pulse (MOPA) nanosecond fibre lasers are sold by several laser companies, including IPG Photonics and SPI Lasers. Q-switched fibre lasers, typically 100 to 150 ns pulse width, are employed for some polymer marking applications, but their repetition rate is limited to around 80 kHz because of the inherent constraint of Q-switching technology.

Directly modulated MOPA (DM-MOPA) fibre lasers operate at repetition rates up to 500 kHz at nanosecond pulse widths. Pulse Width [ns] is a measure of the time between the beginning and end of the pulse, typically based on the full width half maximum (FWHM) of the pulse shape.

High repetition rates generally translate into faster marking speed (in conjunction with other laser/wave form parameters). There are significant differences in wave forms and degree of surface carbonization³ (see Image 1).

Localised spatial and temporal control of the laser heat input and of the rate of heat input enable maximum performance. For temperature-sensitive polymers, variable short-pulse (MOPA) fibre lasers are particularly effective in achieving high contrast without excessive carbonisation.

Subsurface marking is achievable on clear plastics for medical applications. Generally, MOPA lasers generate pulse widths (pulse duration) from 1 ns to 250 ns (and higher). The Sabreen Group has found 20 ns to 50 ns an ideal range for optimal colour contrast in many polymer applications, including nylons.

In cosmetic and functional marking contrast, laser additives make a critical difference when high-resolution, line-edge quality and small data cells are required for direct part marking (DPM) data matrix and bar code. The longer the data string, the more condensed become the data cells.

Grade “A” verification often is required for military, aerospace, automotive and pharmaceutical products. High-contrast code readability has additional benefits – faster marking speeds and low-cost, hand-held readers can be used throughout the factory.

Figure 1. Fixed-pulse vs. MOPA wave forms

Conclusion

Polyamides are among the most challenging polymers to laser mark. Smart laser additives solve contrast problems, increase marking speeds and introduce cost savings. For direct part marking (DPM) data matrix and bar code, laser additives provide critical improvements. Variable short-pulse (MOPA) fibre lasers, 20 ns to 50 ns range, are exceptionally effective in achieving superior contrast colour on most polymers.

References

1. Sabreen, S. Fibre Lasers: Selection and Additives, Plastics Decorating, November 2017. 2. Polyamide (PA) Nylon Complete Guide, SpecialChem 2019. 3. Brodsky, M. Wave Forms: A New Laser Tool, Optics & Photonics, March 2012.

Scott R. Sabreen is founder and president of The Sabreen Group, Inc., an engineering consulting company specialising in secondary plastics manufacturing processes – surface pretreatments, adhesion bonding, inkjet printing, laser marking, decorating and finishing and product security. Sabreen has been developing pioneering technologies and solving manufacturing problems for more than 30 years. He can be contacted at 972.820.6777 or by visiting www.sabreen.com.


Request your free quote

Scott Sabreen — President and Chief Engineer, with over 30 years of expertise. Contact us today to discuss your application and SABREEN solutions free of charge and with no obligation. Bring us your most difficult challenges.

Phone: +1 972-820-6777

Contact us →

Scott Sabreen

Scott Sabreen
President & Chief Engineer
30+ Years of Expertise

Describe your problem in two sentences. Scott Sabreen replies personally, usually within one business day.

Submission Successful!

Thank you. Scott has your message and will reply by email, usually within one business day.

We Have Received Your Request

We have received your request and will be in touch shortly.

🌐 India (English) ▴