Laser Marking of Glass-Filled Polymers – The Importance of Injection Moulding Operations

Plastics laser marking offers numerous advantages across a wide range of industrial applications. Decorative and functional markings produced by the laser must be completely readable, such as component identification, schematics, data matrix and barcode. The quality of the marking depends on the polymer, additives and colourants, injection moulding processes, and the laser source. Moulded polymer surface problems that inhibit readability can affect safety, performance and function of the product. One example is additive glass fibres. The addition of glass fibres can deleteriously affect moulding processes, which in turn affects the quality of laser marking. Resin-rich part surfaces are necessary to achieve robust marking. Surfaces rich in glass fibre will produce inferior results.

Key Takeaways

  • Glass fill typically runs 10–60% across ABS, nylon, acetal, polycarbonate, LCP, PBT, PET, PPS, PEEK and PEI.
  • Fibreglass is not a good near-infrared absorber, so glass-rich surfaces mark poorly by definition.
  • Resin-rich surfaces are the requirement, because the laser energy must interact with the polymer matrix.
  • Glass emergence shows as white marks on the surface after condensation and moulding.
  • Moulding decides markability — the defect originates upstream of the laser, so it must be fixed upstream.

Frequently Asked Questions

What is glass emergence?

A serious surface defect affecting fibreglass-filled injection moulded products, where excess glass forms at the surface during melt filling and moulding. After condensation and moulding, white marks appear on the surface, and the exposed fibres create a glass fibre-rich surface that marks badly.

Why do glass-rich surfaces mark so poorly?

Because fibreglass is not a good absorber of near-infrared laser light. Marking requires the laser energy to interact with the polymer matrix, so surfaces must be resin-rich. The problem worsens as fibre content rises.

Which polymers commonly contain glass fibre?

ABS, nylon, acetal, polycarbonate, liquid crystal polymer, PBT, PET, PPS, PEEK and PEI. Fill percentages vary but typically range between 10 and 60%.

What is fibreglass actually made from?

Silica, limestone and soda ash. Silica forms the glass itself, while soda ash and limestone lower the melting temperature during manufacture.

What are the surface mechanisms that produce a mark?

Three: black marking by carbonisation, white marking by foam generation, and colour change through laser-induced thermal chemical reactions in pigmented polymers. Which occurs depends on the energy absorbed and the material’s unique thermal degradation pathway.

Glass Fibres

When a standard plastic needs to be enhanced for structural performance, glass fibres are added. The improvements in strength result from the weaker polymer transferring load stress to the stronger reinforcing fibres. Materials used to make fibreglass are silica, limestone and soda ash. Silica is the main material used to form the glass while soda ash and limestone are used to lower the melting temperature.

Fibreglass is commonly added to ABS, nylon, acetal, polycarbonate, liquid crystal polymer (LCP), PBT, PET, PPS, PEEK and PEI. Although fill percentages vary, they typically range between 10 to 60%. There are two types of glass reinforcements – short fibre and long fibre – and each has advantages and drawbacks.

Laser Marking of Glass-Filled Polymers – The Importance of Injection Moulding Operations

Glass Emergence Surface Defect

“Glass emergence” is a serious surface defect that commonly affects fibreglass-filled injection moulded products. The exposure of glass fibres causes a glass fibre-rich surface. Excess glass forms on the surface during plastic melt filling and moulding. After condensation and moulding, white marks appear on the surface (see Photo 1).

Moulded part surfaces must be “resin-rich” in order to produce high-quality marking, whereby the energy from the laser interacts with the polymer matrix. Conversely, glass fibre-rich surfaces mark poorly, and the issue gets worse with higher fibre content. Fibreglass itself is not a good absorber of near-IR (NIR) laser light.

The importance of proper injection moulding processes cannot be overstated. Table 1 lists surface defects that can adversely affect the quality of laser markings, in addition to glass emergence.

Table 1. Injection moulding surface defects
Injection moulded writing pen

Polymeric Laser Marking Mechanisms

For NIR beam-steered lasers, 1060-1070 nm wavelength, the mechanism of laser marking involves irradiating the polymer with a localised high-energy radiation source (laser). Laser sources include Ytterbium fibre, Vanadate and YAG. The radiant energy is then absorbed by the material and converted to thermal energy causing reactions in the material to occur. Surface mechanisms for colour change include: 1) black marking by carbonisation, 2) white marking by foam generation, and 3) colour changes by laser-induced thermal chemical reactions of pigmented polymers. The quality of the marking is dependent on the energy absorbed and the materials unique thermal degradation pathway. Each polymer grade, even within the same polymeric family, can produce different results.

For high-quality marking, homogenous distribution/dispersion of colourants and additives is just as crucial as resin-rich surfaces. To determine if distribution/dispersion issues are present, it is recommended to setup the laser to mark/scan continuously across the entire part surface. See Photo 2.

The result shows (left to right) moulded pen displaying excellent gold-on-black chroma marking (left), middle two pictures showing poor chroma distribution and far-right showing excellent uniform distribution.

Since most polymers do not possess NIR absorption properties without chemical additives, experts utilise additives, fillers, pigments and dyes to enhance the absorption of laser energy. Vastly different formulation chemistries and laser optics/setup parameters are used depending upon the desired marking contrast and functionality. Laser additives optimise the degree of contrast and significantly increase marking speed. Both granulate and powder form can be blended into precompounded colour material or colour concentrate. Precolour compounded materials produce more consistent marking versus colour concentrate. The selection of which additive to incorporate depends upon the polymer composition, substrate colour, desired marking contrast colour and end use certification requirements.

Laser marking systems are highly accurate and repeatable. Once the process is set up, the laser will precisely apply and repeat the exact same output energy. Therefore, any surface defects will cause marking inconsistencies.

A challenging application is achieving robust white contrast on blue and black 30% glass-filled polyamide (nylon). See Photo 3.

Laser pulse repetition rate and peak power density are critical parameters in forming the mark and achieving the optimal contrast and speed. The arithmetic curves of power versus pulse repetition rate are inversely proportional.

High peak power at low frequency increases the surface temperature rapidly, vaporising the material while conducting minimal heat into the substrate. As the pulse repetition increases, a lower peak power produces minimal vaporisation, but conducts more heat. Contributing factors that influence the marking contrast and quality are pulse width, focal distance, beam velocity and the vector line separation distance.

Photo 3. Laser marking on resin-rich moulded nylon surface, 30% glass-filled.

Conclusion

In conclusion, plastics laser marking is an excellent process. The quality of marking depends on the polymer matrix, additives and colourants, injection moulding process, and the laser source. Moulded polymer surface issues which inhibit readability can affect safety, performance and function of the product. Glass emergence is one type of moulding surface defects that deleteriously affects the quality of marking. Resin-rich part surfaces and uniform dispersion/distribution are critical to achieving robust laser marking.

Scott R. Sabreen is founder and president of The Sabreen Group, Inc., an engineering consulting company specialising in secondary plastics manufacturing processes – surface pretreatments, adhesion bonding, inkjet printing, laser marking, industrial coatings, decorating and finishing, and product security. He has been developing pioneering technologies and solving manufacturing problems for more than 30 years. He can be contacted at 972.820.6777 or by visiting www.sabreen.com.


Request your free quote

Scott Sabreen — President and Chief Engineer, with over 30 years of expertise. Contact us today to discuss your application and SABREEN solutions free of charge and with no obligation. Bring us your most difficult challenges.

Phone: +1 972-820-6777

Contact us →

Scott Sabreen

Scott Sabreen
President & Chief Engineer
30+ Years of Expertise

Describe your problem in two sentences. Scott Sabreen replies personally, usually within one business day.

Submission Successful!

Thank you. Scott has your message and will reply by email, usually within one business day.

We Have Received Your Request

We have received your request and will be in touch shortly.

🌐 India (English) ▴