Techniques for Measuring Adhesion and Abrasion Durability of Coatings and Inks – Part 1

This is the first of a two-part series on techniques for measuring adhesion and abrasion durability of coatings and inks. This first issue will examine adhesion. Part two will address abrasion durability, including new equipment and measurement techniques.

Adhesion and abrasion durability of cured coatings and inks are two critical performance properties, and their measurement and control are essential for robust manufacturing. Adhesion and abrasion durability are discrete physical properties and commonly misdiagnosed during failure mode analysis. Poor adhesion and abrasion durability are leading causes of field failures, scrap and rework, lower profits, and dissatisfied customers. Techniques exist to measure these properties. This article addresses several different test methods and instruments. Among these is a new linear abraser made by Taber Industries that is designed to evaluate actual product shapes involving contoured surfaces as well as flat specimens (part two). Advanced measurement techniques such as the ones cited in this paper are helping manufacturers achieve superior product performance and six-sigma process excellence.

Key Takeaways

  • Adhesion and abrasion are different properties. A coating can pass one and fail the other, and they are routinely confused in failure analysis.
  • ASTM D3359 is qualitative. It confirms a minimum was met; it cannot quantify bond strength.
  • Tape variability is real — independent labs have recorded differences up to 50% between batches.
  • Both standards were written for rigid substrates, metal and concrete, not for coatings on flexible or semi-rigid plastics.
  • Consistency of procedure matters more than the method chosen. Slight variations produce statistically significant differences.

Frequently Asked Questions

What is the difference between adhesion and abrasion durability?

They are discrete physical properties that are often mutually exclusive. A cured coating can show good adhesion and poor abrasion resistance, or the reverse. Identifying which mechanism actually failed — adhesion, cohesion, abrasion or a combination — determines the engineering fix.

Is the ASTM D3359 tape test reliable?

It is simple, cheap and widely used, but qualitative. It establishes that a minimum adhesion value was met rather than measuring actual bond strength, and accuracy is operator dependent by design since no calibrated equipment is required. It was also developed for ductile coatings on metal, not for plastics.

Why do tape test results vary between labs?

Tape. Batches have inherent adhesion variability, and independent laboratories have noted differences of up to 50%. The original 3M 710 tape was discontinued and Permacel changed its tape properties over time, which effectively opened the test to any pressure-sensitive tape.

When should I use ASTM D4541 pull-off testing instead?

When you need a quantitative tensile result. Be aware it typically requires product sizes of three inches or larger to accommodate standard dollies, needs testing in at least two or three locations, and that fixed-alignment, hydraulic and pneumatic instruments give results that vary considerably — direct comparison between them is impractical.

How should the dolly be prepared for a pull-off test?

Machined or end-milled dolly faces typically yield weaker bonds. Lightly roughen the surface with a Scotch-Brite pad or sandpaper to create microstructure, then clean with alcohol and a dry cloth to remove grit, oils and oxidation. Use an adhesive that will not interact with the coating.

Adhesion versus Abrasion

Optimal adhesion and abrasion durability (resistance) of cured coatings and inks onto plastic substrates must be achieved during manufacturing to produce high quality products that will endure throughout their service life. These properties can be interdepen- dent but often are mutually exclusive. That is, cured coatings and inks can demonstrate good adhesion and poor abrasion, or poor adhesion and good abrasion. Proper testing and understanding of adhesion and abrasion ensures conformance to specifications and is invaluable in solving coating and printing problems. The identification of the failure mechanism, adhesion (cohesion), abrasion or both, will determine the engineering process solution. Historical test methods and new instrumentation exist to measure and analyse these properties.

Adhesion Test Methods

ASTM D 3359 Standard Test Method for Measuring Adhesion by Tape Test is historically perhaps the most well-known and widely used method for testing adhesion of coatings and inks because of its simplicity and low cost. The most basic procedure for conducting the tape test includes the following:

  • Agreement on the selection of tape.
  • Complete cure of the coatings and inks before testing.
  • Making “X”-cuts in the film per Method A or lattice pattern with either six or eleven cuts in each direction per Method B.
  • Removing and discarding two laps of tape from the roll dispenser.
  • Smoothing the tape into place by finger and then rubbing firmly with an eraser on the end of a pencil, or similar (the colour under the tape being a good indicator of complete contact).
  • Within 60-120 seconds of application, removing the tape by pulling the free end rapidly (not jerked) back upon itself as close to an angle of 180 degrees as possible.
  • Inspecting the cut area for removal of coating from the substrate and rating the adhesion relative to pre-determined descriptions and illustrations classifications (0B, 1B, 2B, 3B, 4B, 5B).

Early versions of ASTM D 3359 referenced the use of 3M 710 and Permacel tape. 3M discontinued its product, and over the years, Permacel changed the properties of its tape. The ASTM subcommittee advised users to check whether the current Permacel gives comparable results to the original tape. This proved to be impractical and opened the floodgates for companies to use virtually any type of pressure-sensitive tape. Many companies today use abbreviated versions of ASTM D 3359, in which specific product niches are tested as similarly as possible, e.g., cellular phones, computer keyboards, automotive components, etc. Several commonly used techniques and pressure-sensitive tapes are shown.

There are important considerations to keep in mind when conducting the tape test so that repeatable and reproducible results can be achieved to determine acceptable or unacceptable adhesion without bias. Batches (rolls) of tape as manufactured have inherent adhesion variability, especially over time. For example, independent laboratories have noted differences of up to 50 percent. The tape test is qualitative and cannot precisely assess quantitatively the actual strength of the adhesive bond (only a minimum value was met). However, it does provide relative adhesion performance. The test method was originally developed for ductile coatings applied to metal substrates and not for coatings or inks applied to plastic products.

Tape Resin Adhesion to Steel Manufacturer
Scotch 600 Transparent Acrylic 25 oz/in 3M
Scotch 610 Cellophane Rubber 43 oz/in 3M
Scotch 810 Magic Tape Acrylic 25 oz/in 3M
Lithographers 616 Tape Rubber 36 oz/in 3M
Scotch 893 Filament Tape Rubber 55 oz/in 3M
Permacel 99 Rubber 52 oz/in Nitto Denko
The cross-hatch adhesion test kit laid out: a roll of pressure-sensitive tape, a cross-hatch cutter, a brush, a cutting blade and a magnifier.
Illustration of a multi-blade cross-hatch cutter drawing a lattice of evenly spaced parallel cuts through a coating.

The cross-cut test is a simple and easily predictable method for evaluating the adhesion of single- or multi-coat systems.

Procedure

  • Make a lattice pattern in the film with the appropriate tool, cutting to the substrate
  • Brush in diagonal direction 5 times each, using a brush pen or tape over the cut and remove with Permacel tape
  • Examine the grid area using an illuminated magnifier

Cross-Cut Results

Adhesion is rated in accordance with the scale below:

Standards
ASTM D 3002 D 3359
DIN EN ISO 2409
Cross-hatch adhesion test specimen rated ISO Class 0 / ASTM Class 5B: the cut edges are completely smooth and no squares of the coating have detached.
Cross-hatch adhesion tape test result rated ISO Class 1 / ASTM Class 4B, showing slight flaking at the lattice intersections, with a schematic of the cut grid alongside.
Cross-hatch adhesion test specimen rated ISO Class 2 / ASTM Class 3B: flaking along the cut edges and at the lattice intersections.
Cross-hatch adhesion test specimen rated ISO Class 3 / ASTM Class 2B: the coating has flaked away along the cuts in ribbons and whole squares are partly detached.
Cross-hatch adhesion test specimen rated ISO Class 4 / ASTM Class 1B: large ribbons of coating have lifted and whole squares have detached.
Label reading ISO Class 5 / ASTM Class 0 B, the lowest cross-hatch adhesion rating on the scale.

*DIN 53151 was withdrawn in October 1994

Thus, when a flexible adhesive tape is applied to a flexible or semi-rigid plastic, rather than a rigid metal, the peel phenomenon and failure mechanisms are different

Differences in tapes, backing stiffness, and adhesive theology can yield different results even on the same product tested. A given tape formulation inherently does not adhere equally to all coatings and plastics. Surface texture is also an important factor. ASTM D 3359, by design, was made to be simple and not require calibrated equipment. Thus, the test accuracy is operator dependent.

ASTM D 4541 Standard Test Method for Pull-Off Strength of Coatings Using Portable Adhesion Testers is also a well-known standard. Unlike ASTM D 3359, however, it requires the use of instrument apparatus referred to as pull-off adhesion testers. Several different instrument apparatus models are cited (fixed alignment, hydraulic, pneumatic) and may yield different results depending upon the instrument parameters and usage. The tensile adhesion test determines either the greatest perpendicular force (in tension) that a surface area can bear before any material is detached or whether the surface remains intact at a predetermined force (pass/fail). Results from extensive industry test- ing with the three models on identical surfaces vary considerably, making direct comparison impractical.

Regardless of which pull-off adhesion tester is used, the procedure begins with securing a loading fixture (termed “Dolly”) perpendicular to the surface of the coating with an adhesive. After the adhesive is cured, a testing apparatus is attached to the loading fixture and aligned to apply tension normal to the test surface. The force applied to the loading fixture is gradually increased until either material detachment “pull-off” occurs or the specified value is achieved.

When multiple coatings are applied, the nature of the failure mechanism, adhesive or cohesive failure, will be derived. Two examples of the many devices commercially available are shown below. Figures A and B show the Elcometer 106 Fixed Alignment apparatus and figures C and D show the Defelsko Hydraulic Self-Aligning apparatus.

Pull-off adhesion tester kit: pressure gauge, hydraulic pump and hose, test dollies and fittings.
Labelled cross-section of a pull-off adhesion test fixture, identifying the detaching assembly, central grip, loading fixture, annular ring, adhesive, base and coating system.

For any of the pull-off adhesion testers, surface preparation of the dolly and application of adhesive is important to achieving accurate, reproducible results. Many dollies, as purchased, have smooth machined and/or end milled surfaces, however they typi- cally yield weaker bonds. Some users of pull-off adhesion testers may modify the dolly surface using either Scotch-Brite® pad or sandpaper to provide a slightly roughened surface, creating microstructures for maximum bond strength. After “dressing” the dolly, it must be cleaned (usually alcohol and dry cloth) to remove excess grit, oils, and oxidation. A common adhesive used is Araldite 2011, a two-component epoxy that may require up to 24 hours to cure before the pull test can be conducted. Other adhesives can be selected, but it is paramount that the adhesive not affect or interact with the coating, or the test results will be of minimal value.

Regardless of the pull-off adhesion tester selected for use, the most critical aspect of conducting this test is the consistency of how the test is conducted. Even slight variations in procedure will cause statistically significant data results. Many users of this test method use disposable aluminium dollies. Documented procedures will help minimise variation as a result of inconsistent setup.

ASTM D 4541 was also developed for the specific purpose of testing coatings on rigid structures such as metal, concrete, or wood. Unlike ASTM D 3351, that can be conducted on relatively small parts, ASTM D 4541 typically requires product sizes of three inches or larger to accommodate standard dolly sizes (although custom dollies can be purchased). ASTM D 4541 procedure should be conducted in at least 2-3 locations on a part, which can make it impractical for small products. The decision to use ASTM D 3351, ASTM D 4541, or other adhesion tests is up to each company and may be influenced by historical testing conducted within its market niche.

Test Standards and Process Excellence

Many companies use some of the test methods discussed in this paper out of necessity, i.e., to acquire business by demonstrating their manufacturing processes conform to specific industry standards. Unfortunately, manufacturers can often be unaware of field failure problems until their customers return nonconforming products. By default, “poor adhesion” is to blame. Through proper understanding of the many possible causes for adhesion versus abrasion failures, engineers can adroitly identify the critical root causes and implement corrective actions. Testing should not be reserved only for product development and troubleshooting. Continuous in-line testing of products using the methods and techniques presented and Six Sigma techniques will ensure robust manufacturing.

Acknowledgements

  • 3M Corporation Industrial Tape & Specialties
  • Division American Society of Testing and Materials International
  • BYK Gardner
  • Defelsko Corporation
  • Elcometer Inc
  • Gardner Company
  • Permacel (Nitto Denko Company)

Scott R. Sabreen is founder & president of The Sabreen Group, Inc. (TSG). TSG is a global engineering company specialising in secondary plastics manufacturing processes – surface pretreatments, bonding, decorating & finishing, laser marking, and product security. For more information, call toll-free (888) SABREEN or visit: www.sabreen.com.


Request your free quote

Scott Sabreen — President and Chief Engineer, with over 30 years of expertise. Contact us today to discuss your application and SABREEN solutions free of charge and with no obligation. Bring us your most difficult challenges.

Phone: +1 972-820-6777

Contact us →

Scott Sabreen

Scott Sabreen
President & Chief Engineer
30+ Years of Expertise

Describe your problem in two sentences. Scott Sabreen replies personally, usually within one business day.

Submission Successful!

Thank you. Scott has your message and will reply by email, usually within one business day.

We Have Received Your Request

We have received your request and will be in touch shortly.

🌐 India (English) ▴