How to Laser Mark and Engrave Nylon (Polyamide) Plastics with Fibre Lasers

Abstract

Users of fibre lasers have difficulty marking or engraving nylon. The key to achieving high–quality marking contrast is to incorporate laser enhancing additives into the nylon material during the moulding process, whether using colour concentrate or precompounded materials. The benefits of laser marking nylon have transformed many industries, including firearms by enabling unique part identification, data matrix and QR codes, and customisation.

Key Takeaways

  • Unmodified nylon marks poorly. Polyamide absorbs little energy at 1060–1070 nm, so contrast depends on laser additives.
  • The best contrast pairs are opaque white on black, jet black on white, and opaque white on medium blue.
  • MOPA ytterbium fibre lasers are the right tool; pulse widths below about 90 ns suit plastics.
  • Loading runs 0.01–3.0% by weight, and uniform dispersion through every part is what makes contrast repeatable.
  • Glass-filled nylon is harder still — fibre-rich surfaces mark badly, so resin-rich surfaces are essential.
White laser marking on blue background
White laser marking on black background

Nylon plastics have a wide range of applications including firearms, automotive, electrical & electronics, industrial, consumables and oil & gas. However, the varying physical, chemical, and surface properties of nylon (polyamide), particularly glass-filled nylons, make laser marking & engraving challenging. The most popular contrast colours are opaque white on black, jet black on white, and opaque white on medium blue. When laser additives are combined with the appropriate pigments and dyes, they produce superior marking quality at a low cost. Laser additives are used in a variety of plastics, including ABS, Acetal, PET, PVC, polycarbonate, polypropylene, and polyethylene.

Nylon Polyamides

Polyamides, also known as nylon, are a prominent class of thermoplastics used in high-performance applications. They consist of amide linkages, specifically –CO-NH–. Nylon is synthesized through the process of polycondensation, wherein a diamine reacts with a diacid, or through ring-opening polymerisation of lactams containing six, eleven, or twelve carbon atoms. Nylon monomers can be aliphatic, semi-aromatic or aromatic (aramids) and can range in structure from amorphous, semi-crystalline and of greater or lesser crystallinity. Two major polyamides are poly(hexamethylene adipamide) (nylon 6,6) and polycaprolactam (nylon 6). Aliphatic polyamides include nylon 12, 69, 6-10, 6-12, 46 and 1212. The bio-based engineering plastic known as Nylon 11 is sourced from renewable resources, specifically castor plants.

Laser Marking Surface Mechanisms

Laser-markable plastics are characterised by their ability to absorb laser light and subsequently convert it into thermal energy within the near-infrared (NIR) range of wavelengths between 1060nm-1070nm. Three common types of lasers are Ytterbium fibre (MOPA & Fixed pulse), Vanadate (Nd:YVO4), and Nd:YAG. Depending on the type of laser and the desired marking contrast, a variety of chemistries can be used to produce surface reactions such as carbonisation charring, chemical change foaming, and colour change. The same laser can perform all surface reactions by adjusting the settings in the marking software (power, pulse repetition rate, and marking speed). Continuous wave (CW) CO2 lasers have a wavelength of 10.6 microns (far infrared spectrum). CW CO2 lasers have lower peak power and cannot produce high contrast markings on plastics.

Laser Additives

Since most polymers have limited absorption properties in this wavelength (NIR) and cannot produce noticeable contrast, experts use a variety of additives, fillers, pigments, and dyes to increase absorption and achieve high contrast quality. Additives increase the degree of colour contrast (absorption of laser light), which is further enhanced by optimal laser selection and marking parameters. Unlike popular belief, there isn’t a single universal additive.

Some additives contain antimony-doped tin oxide and antimony trioxide mixtures, which can cause the natural (uncoloured) substrate opacity to appear “grayish”. Other additives may contain aluminium particles, mixed metal oxides, or proprietary compounds. Colour adjustments are made with pigments and dyes to achieve the desired colourmatch appearance. Specific additives have been approved by the FDA for use in food contact and food packaging under conditions A-H of 21 CFR 178.3297 Colourants for Polymers.

Laser additive compounds are available in pellet granulate and powder form. Granulate products are blended directly with the polymer resin, while powder forms are converted into masterbatch. The loading concentration level by weight (in the final part) usually ranges between 0.01 and 3.0%. To achieve the best colour contrast, laser additives must be distributed/dispersed uniformly throughout each part.

Fibre Lasers

Nanosecond Ytterbium fibre lasers (MOPA and Fixed pulse) are ideal for marking, engraving, and etching plastics due to their superior beam quality (M2) and high brightness “radiance”. They can focus to a small spot size (less than 20 microns), resulting in high energy density. One significant advantage of using MOPA (Master Oscillator Power Amplifier) lasers is ability to fine tune the pulse width. Low pulse width, typically less than 90 nanoseconds, is ideal for marking plastic materials.

Laser irradiance (W/cm2) and fluence (J/cm2) are important parameters in plastic marking. The intensity is influenced by pulse frequency, laser power, focal spot size and pulse width. Fluence is influenced by beam intensity, scan velocity, pulse overlap, and focus beam diameter. Pulse repetition rate and peak power density are critical parameters in forming the mark and achieving the optimal contrast and speed. High peak power at low frequency increases the surface temperature rapidly, vaporising the material while conducting minimal heat into the substrate. As the pulse repetition increases, a lower peak power produces minimal vaporisation but conducts more heat. The arithmetic curves of power versus pulse repetition rate are inversely proportional.

Frequently Asked Questions

Why will my fibre laser not mark nylon clearly?

Polyamide has limited absorption in the near-infrared band where ytterbium fibre lasers operate, so most of the energy does not convert into the thermal reaction that forms a mark. The fix is a laser-enhancing additive compounded into the material, not more laser power.

What additives are used for laser marking nylon?

Antimony-doped tin oxide and antimony trioxide mixtures are common, though they can give uncoloured substrates a greyish cast. Others use aluminium particles, mixed metal oxides or proprietary compounds, with pigments and dyes added to hit the final colour match.

Can laser-marked nylon be used for food-contact parts?

Yes, with the right additive. Specific additives are approved by the FDA for food contact and food packaging under conditions A–H of 21 CFR 178.3297, Colourants for Polymers. Confirm the approval covers your grade and loading.

What pulse width should I use on nylon?

Short pulses. On a MOPA laser, widths below roughly 90 nanoseconds suit plastics, delivering high peak power that raises surface temperature quickly while conducting minimal heat into the substrate.

Why is glass-filled nylon harder to mark than unfilled?

Glass fibres do not absorb near-infrared and they scatter the beam, so fibre-rich surfaces mark weakly and inconsistently. Moulding must be tuned to produce resin-rich surfaces. See glass fibre emergence and laser marking.

Scott R. Sabreen is founder and president of The Sabreen Group, Inc., which is an engineering company specialising in secondary plastics manufacturing processes – surface pretreatments, bonding decorating and finishing, laser marking and product security. He has been developing new technologies and solving manufacturing problems for over 30 years. Sabreen can be contacted at 972.820.6777 or by visiting www.sabreen.com or www.adhesionbonding.com.


Request your free quote

Scott Sabreen — President and Chief Engineer, with over 30 years of expertise. Contact us today to discuss your application and SABREEN solutions free of charge and with no obligation. Bring us your most difficult challenges.

Phone: +1 972-820-6777

Contact us →

Scott Sabreen

Scott Sabreen
President & Chief Engineer
30+ Years of Expertise

Describe your problem in two sentences. Scott Sabreen replies personally, usually within one business day.

Submission Successful!

Thank you. Scott has your message and will reply by email, usually within one business day.

We Have Received Your Request

We have received your request and will be in touch shortly.

🌐 India (English) ▴