Cold Gas Plasma Surface Modification – Optimise Plastics Bonding Adhesion

Cold Gas Plasma Surface Modification – Optimise Plastics Bonding Adhesion

Key Takeaways

  • It is the only common method that treats PTFE successfully.
  • Typical parameters: 5–10 minutes, 100–500 sccm gas flow, 300–1000 mTorr, 200–1000 W RF, 75–125°F.
  • It removes hydrocarbons, which can eliminate a separate solvent cleaning step that atmospheric methods still require.
  • Activation lasts significantly longer and treats more uniformly than atmospheric methods.
  • “Batch only” is a myth. Reel-to-reel continuous treatment of web materials runs inside the chamber.

Polymeric and elastomeric substrates can be extremely challenging to achieve robust bonding adhesion strength to like or dissimilar materials. Bonding applications are not limited to only adhesives, but include printing inks, paints and coatings, encapsulant and potting compounds, metallisation and more. This article describes “Low Pressure Cold Gas Plasma” surface modification as one type of process that can resolve many three-dimensional bonding problems through plasma chemical surface activation and functionalisation. The science of well known “atmospheric or air” surface modification processes will be compared.

Particularly notorious tough-to-bond substrates include silicone and rubber elastomers and engineering thermoplastics including acetals, fluropolymers, polyolefins, nylons, polycarbonates, polyesters, styrenics, and more. The underlying reasons why many plastics and elastomers are difficult to bond are that they are hydrophobic non-polar materials, chemically inert, and possess poor surface wettability (i.e., low surface energy).

Frequently Asked Questions

What makes cold gas plasma different from atmospheric plasma?

It runs in an enclosed evacuated chamber rather than in open air. A selected gas — commonly industrial-grade oxygen, but also argon, nitrogen, ammonia or fluorine — is released under partial vacuum and subjected to an RF or microwave field, giving precise control over the reactive species.

Can cold gas plasma treat PTFE?

Yes, and it is unique among the common methods in doing so successfully. It can also grow polymer coatings on surfaces through plasma-enhanced chemical vapour deposition, producing conformal SiO2-like and diamond-like coatings up to about 2 µm.

What process parameters should I expect?

As general guidelines: total treatment time 5 to 10 minutes, gas flow 100 to 500 sccm, pressure 300 to 1000 mTorr, RF power 200 to 1000 watts, and low process temperature between 75 and 125°F. Exact values depend on the specific system.

Is cold gas plasma limited to offline batch processing?

No — that is a frequently repeated misnomer. Reel-to-reel continuous treatment of woven polymeric fabric web materials runs continuously within the chamber, and chamber dimensions permit high-volume treatment of both small and large parts.

When is cold gas plasma worth its higher cost?

When you need the most robust result, the longest activation life, or treatment of substrates such as PTFE that atmospheric methods cannot handle. It also removes hydrocarbons, which can eliminate a separate solvent cleaning step. Atmospheric treatments are cheaper but can suffer day-to-day humidity variation affecting uniformity.

What Is Plasma?

Plasmas can be conceptualised as a fourth state of matter. As energy is supplied, solids melt into liquids, liquids vaporise into gases, and gases ionise into “plasmas” – an extremely reactive gas. Free electrons, ions, metastables, radicals, and UV generated in the plasma can impact a surface with energies sufficient to break the molecular bonds on the surface of most polymeric substrates. This creates very reactive free radicals on the polymer surface which, in turn, can form, cross-link or – in the presence of oxygen – react rapidly to form various chemical functional groups on the substrate surface. Polar functional groups that can form and enhance bondability include carbonyl (C=O), carboxyl (HOOC), hydroperoxide (HOO-), and hydroxyl (HO-) groups. Even small amounts of reactive functional groups incorporated into polymers can be highly beneficial to improving surface chemical functionality and wettability.

Cold Gas Plasma Surface Modification

In comparison to atmospheric (air) surface pretreatment methods, “low pressure cold gas plasma” surface modification is conducted in an enclosed evacuated chamber. Industrial-grade oxygen gas (O2) commonly is used in plastics pretreatment applications. Other oxidising and noble gases include argon, nitrogen, ammonia NH3, fluorine, and combinations thereof. The selected gas to be ionised into the reactive gas plasma is released into the chamber under a partial vacuum and subjected to an electrical field (RF or MW).

It is the response of the highly reactive species generated with the polymers placed in the plasma field, on inner conductive electrode aluminium shelves or cage, breaking molecular bonds that results in chemical/physical surface modifications without affecting the bulk substrate properties. Cold gas plasma process modifies non-wettable hydrophobic surfaces to bondable hydrophilic wettable surfaces via chemical and physical mechanisms. See Diagram 1.

Micro nano-scale roughened surfaces can be selectively altered in the plasma environment either by a bombarding effect of ions accelerated toward the surface, or by a chemical etch process. Roughened surfaces have higher surface areas (peaks and valleys), equating to a higher number of binding sites that improve bonding adhesion. See Diagram 2.

Unique to the cold gas plasma is that it successfully can pretreat PTFE. Further, polymer coatings can be grown on surfaces through a process called plasma-enhanced chemical vapour deposition (PECVD). Coatings are highly conformal with thickness (?2µ) dependant on process time.

Examples of coatings include SiO2-like and Diamond-like. A key application is to coat the insides of plastic and glass tubes and containers with a quartz-like material that acts as a barrier to leachables and prevents breakage.

Cold Gas Plasma - The Sabreen Group, Inc.

Equipment System Set-Up

Low pressure cold gas plasma system equipment consists of a vacuum chamber made of aluminium with a hinged door for loading and unloading parts. All systems have similar important component features including vacuum pump, RF generator, MFC (Mass Flow Controller), and microprocessor controller.

The parts to be cleaned are simply placed on the inner electrodes which are removable shelves or a cage. The parts/shelves subsequently are loaded into the reaction chamber in which the process begins by first pumping down to a vacuum.

The process gas then may flow through the system at a regulated pressure while pumping continues. The RF generator supplies excitation power. At the end of the plasma process the closed vacuum chamber returns to ambient pressure, whereby the treated parts are removed and ready for bonding. Most systems allow for automatic control of process variables including (typically) pressure, power, gas flow, temperature, and cycle times (intermediary stage and total elapsed time). See Diagram 3.

Processing Control Parameters

Operating process parameters are based upon specific manufacturer model system specifications. Thus, it is important to understand the application requirements for improved bondability, production throughput, and downstream manufacturing processes to maintain the treatment shelf-life (aging) and contamination sources within the work environment. As general guidelines, total cold gas plasma treatment time will range between 5-10 minutes; gas flow 100-500 sccm; pressure 300-1000 mTorr, RF power 200-1000 Watts; and low temperature heat during processing 75-125°F.

Misnomers of Cold Gas Plasma Pretreatment

It is frequently cited that cold gas plasma treatment is an “inefficient” method, limited to only off-line batch processing, compared to atmospheric plasma methods. This is false. Reel-to-reel continuous treatment of woven polymeric fabric web materials, e.g., threaded polypropylene baby diaper fabric, is treated continuously within the chamber. Based upon the inside chamber dimensions, cold gas plasma processes can treat high-volume small and large parts. While manufacturing process operations can be most efficiently performed in-line, many product assemblies are conducted in batch or cell manufacturing.

Gas-Phase Surface Oxidation Pretreatments

Surface oxidation modification vis-à-vis surface pretreatments is used to improve the wettability and bondability of polymers and elastomers both chemically and physically. Well known process methods are electrical (corona discharge) and flame plasma. Historically, low pressure cold gas plasma has been less practiced and discussed for the pretreatment of three-dimensional parts, due in part to misnomers of the process. In the science of chemistry and physics, electrical, flame, and cold gas plasma are all “Gas-Phase Surface Oxidation Processes” characterised by their ability to generate a “gas plasma.” The mechanism of how the plasmas are generated is a distinguishing factor. Each method can be application-specific and each possesses advantages and limitations.

Atmospheric Surface Modification Systems

In contrast to cold gas plasma, which is conducted in a low pressure vacuum chamber, flame treatment and electrical (corona discharge) pretreatment processes are conducted at atmospheric conditions. Electrical treatments are further distinguished as “blown air” plasma and “blown ion.” Atmospheric processes can be used in both batch and continuous line production. In terms of nomenclature it is important to understand the science of each process.

Flame Plasma Treatment uses the highly reactive species present in the combustion of air and hydrocarbon gas (to create the plasma). Flame treatment is exothermic; however, heat does not create the chemical functionality and improved surface wetting. Flaming will clean dirt, debris, and some hydrocarbons from the substrate. Flaming will not remove silicones, mould releases, and slip agents. Flame treatment can impart higher wetting, oxidation, and shelf-life than electrical pretreatments due to its relative shallower depth of treatment from the surface, 5-10nm. Ozone is not produced2.

Classical Electrical Corona Discharge is obtained using a generator and electrode(s) connected to a high voltage source, a counter electrode at potential zero, and a dielectric used as a barrier. That is, high frequency-high voltage discharge (step up transformer) creating a potential difference between two points requiring earth ground 35+kV and 20-25kHz. This pretreatment process has virtually no cleaning capabilities. Ozone (NOx) is produced.

Electrical “Air Plasma” is Corona discharge spot treatment (also termed blown air plasma/forced air corona/blown arc). This treatment head consists of two hook electrodes in close proximity to each other connected to a high voltage transformer generating an electric arc of approximately 7-12 kV, lower frequency 50-60 cycles/sec (relative to electrical corona discharge). Then using forced air, a continuous electric arc produces a corona discharge, “plasma.” No positive ground needed. This pretreatment process has virtually no cleaning capabilities. Ozone is produced.

Electrical Blown ion plasma also is termed Focused Corona plasma/Potential-free plasma. This treatment utilises a single narrow nozzle electrode, powered by an electrical generator and step-up transformer and high pressurised air in which an intense focused plasma is generated within the treatment head and streams outward. Since the process is potential-free, it can be used to pretreat conductive products. This pretreatment process can clean dirt, debris, and some hydrocarbons from the substrate but not most silicones and slip agents. New research indicates that fine etching of the surface can create new topographies for increased mechanical bonding. Ozone is not a byproduct.

UV radiation/Ozone pretreatment and chemical primers also are performed at atmospheric conditions. These pretreatment methods will be discussed in a future article.

Factors Influencing Adhesion and Aging

The degree or quality of pretreatment for strong adhesion strength is affected by the cleanliness of the plastic/elastomeric surfaces. Contamination sources on product surfaces that inhibit treatment include dirt, dust, grease, and oil. Low molecular weight materials such as silicones, mould release, and anti-slip agents are particularly deleterious for bonding. Further, certain soluble or nonsoluble compound agents used in pigment and dye colourants can adversely affect adhesion. Exposure of treated surfaces to elevated temperatures increases molecular chain mobility. The higher the chain mobility is, the faster the aging of the pretreatment.

Plasma-treated surfaces age at different rates and to varying extents relative to factors with the surrounding environment. Aging characteristics and their storage shelf-life are essential to manufacturing process operations. Activated surfaces may have a shelf-life of hours, days, months, or longer. The cold gas plasma process demonstrates significantly extended activation lifetimes3 and more uniform treatment compared to atmospheric methods4. It is recommended to bond, coat, paint, or decorate products as soon as possible following pretreatment.

The global need to achieve robust bonding adhesion on plastic and elastomeric products demands surface modification “activation” pretreatments. Chemical and physical functionality and surface roughening, via gas phase surface oxidation processes, can resolve most adhesion problems. Each method can be application-specific and may possess unique advantages and/or limitations. Plasma-oxidised surfaces can deleteriously affect downstream assembly processes, such as poor heat sealing/welding, when overtreatment occurs. While cold gas plasma is the most expensive method, in some applications it has the capability to yield the most robust results. Atmospheric treatments are lower cost. However in some cases, day-to-day humidity variation can affect the treatment uniformity. Careful evaluation of all process factors and an understanding of the alternative surface modification technologies are important.

References

  • Demetrius Chrysostomou, PVATepla, March 2009
  • Scott R. Sabreen, Joe Digiacomo, Plastics Decorating Magazine
  • Edward M. Liston, GaSonics International, Journal of Adhesion 1988
  • Dori & Kushner, University of Illinois and 3M

Scott R. Sabreen is founder and president of The Sabreen Group, Inc. (TSG). TSG is a global engineering company specialising in secondary plastics manufacturing processes ? surface pretreatments, bonding, decorating and finishing, laser marking, and product security. For more information, call (888) SABREEN or visit www.sabreen.com or www.plasticslasermarking.com.


Request your free quote

Scott Sabreen — President and Chief Engineer, with over 30 years of expertise. Contact us today to discuss your application and SABREEN solutions free of charge and with no obligation. Bring us your most difficult challenges.

Phone: +1 972-820-6777

Contact us →

Scott Sabreen

Scott Sabreen
President & Chief Engineer
30+ Years of Expertise

Describe your problem in two sentences. Scott Sabreen replies personally, usually within one business day.

Submission Successful!

Thank you. Scott has your message and will reply by email, usually within one business day.

We Have Received Your Request

We have received your request and will be in touch shortly.

🌐 India (English) ▴